Young's modulus of common materials
Young's modulus E in GPa: the stress it would take to stretch the material to twice its length if it held. Alloys, wood, concrete and plastics vary with composition and manufacture, so those rows are typical values. Wood is along the grain.
| Material | Temperature (°C) | E (GPa) |
|---|---|---|
| Diamond | not stated by the source | 1,220 |
| Tungsten | 20 | 411 |
| Stainless steel | 20 | 215.3 |
| Mild steel | 20 | 211.9 |
| Iron (soft) | 20 | 211.4 |
| Cast iron | 20 | 152.3 |
| Copper | 20 | 129.8 |
| Titanium | 20 | 115.7 |
| Brass (70 % Zn, 30 % Cu) | 20 | 100.6 |
| Fused quartz | 20 | 73.1 |
| Crown glass | 20 | 71.3 |
| Aluminium | 20 | 70.3 |
| Granite | not stated by the source | 52 |
| Bone (compact) | not stated by the source | 18 |
| Concrete | not stated by the source | 17 |
| Lead | 20 | 16.1 |
| Scots pine, along the grain | not stated by the source | 16 |
| Oak, along the grain | not stated by the source | 11 |
| Balsa, along the grain | not stated by the source | 6 |
| Polycarbonate | 20 | 2.4 |
| Polyethylene (HDPE) | not stated by the source | 0.8 |
| PTFE (Teflon) | 20 | 0.4 |
Download the table
The CSV uses commas between fields and a decimal point. In the Excel file the numbers are plain numbers, which Excel shows in your own format.
Sources
(2)
- The Engineering ToolBox, Young's Modulus, Tensile Strength and Yield Strength Values for some Materials (The Engineering ToolBox (2003)) — checked October 1, 2026
- Kaye & Laby, Tables of Physical and Chemical Constants (NPL), §2.2.2 Elasticities and strengths (Version 1.0 content (site last updated 2017), Internet Archive copy of 2018-12-16) — checked October 1, 2026